Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Intergranular corrosion (IGC) bend testing is a widely accepted qualitative method for evaluating the susceptibility of stainless steels to grain boundary attack caused by sensitization. The test combines immersion of specimens in a boiling corrosive medium with a subsequent bend test to reveal intergranular cracks, in accordance with international standards such as ASTM A262, ISO 3651, and GB/T 4334. This article provides a comprehensive technical overview of the testing principle, sample requirements, test procedures, evaluation criteria, and typical industrial applications.

Technical Overview

Intergranular corrosion is a localized form of corrosion that preferentially attacks the grain boundaries of metals while leaving the grain interiors largely unaffected. In stainless steels, this phenomenon is primarily caused by sensitization — a metallurgical condition that occurs when the material is exposed to temperatures between approximately 425 °C and 815 °C, typically during welding, slow cooling after heat treatment, or prolonged service at elevated temperatures.

During sensitization, chromium carbides (Cr23C6) precipitate at the grain boundaries, depleting the adjacent regions of chromium to levels below the approximately 12% required for passivation. These chromium-depleted zones become electrochemically active and are preferentially dissolved when exposed to specific corrosive media. The result is a severe loss of cohesion between grains, deterioration of mechanical properties, and an increased risk of brittle fracture, even though the material may appear visually intact.

The intergranular corrosion bend test is a screening and acceptance method in which a sensitized specimen is first exposed to a boiling test solution that selectively attacks chromium-depleted grain boundaries, and then subjected to a bend test. The presence of intergranular cracks, fissures, or delamination on the tension surface of the bent specimen indicates susceptibility to intergranular attack. This method is specified in major international standards, including ASTM A262 (Practices A through F for austenitic stainless steels), ASTM A763 (for ferritic stainless steels), ASTM G28, ISO 3651-1 and ISO 3651-2, EN ISO 3651-2, and GB/T 4334.

Testing Samples

Test specimens shall be representative of the product form and its metallurgical condition. Surface preparation, dimensional tolerances, and the removal of any oxide scale or cold-worked layer are essential to ensure valid and reproducible results. Typical sample types include:

Plates, Sheets, and Strips

Flat specimens are cut to dimensions specified by the relevant standard, commonly with a width of approximately 10 mm to 30 mm and a thickness of 3 mm to 5 mm. For thin sheet materials, several layers may be tested simultaneously, provided that bending is performed on each layer individually or the standard permits stack testing. Specimens are usually taken in both the longitudinal and transverse directions when product anisotropy is of concern.

Pipes and Tubes

Specimens may be full cross-section rings, longitudinal strips flattened prior to testing, or curved segments. For welded pipes, specimens must include the weld seam, heat-affected zone (HAZ), and base metal so that the sensitized regions produced by welding thermal cycles are properly evaluated.

Forgings and Castings

Specimens are machined from locations most likely to experience sensitization or from regions critical to service performance. Castings may exhibit coarse grain structures and segregation, so sampling locations should be agreed upon between the purchaser and the accredited third-party laboratory performing the test.

Bars, Rods, and Wires

Small-diameter bars and wires may be tested in full section, while larger sections are machined into rectangular strips. Bend testing of wires is often performed by winding around a mandrel of specified diameter.

Welded Joints and Weld Metal

Weldment specimens are prepared transverse to the weld so that the bend test simultaneously evaluates the weld metal, fusion line, and heat-affected zone. This is particularly important for austenitic stainless steels welded without low-carbon or stabilized consumables, where the HAZ is most vulnerable to sensitization.

Testing Items

The intergranular corrosion bend test encompasses several linked testing items that together determine whether a material is susceptible to intergranular attack:

  • Sensitizing heat treatment (where specified): applying a defined heat treatment, such as 650 °C for 30 minutes followed by water quenching, to amplify any inherent susceptibility before corrosion exposure.
  • Corrosion immersion test: boiling the specimen in a standardized aggressive solution for a defined duration to selectively attack chromium-depleted grain boundaries.
  • Bend test: bending the corroded specimen through a specified angle (typically 180°) around a mandrel of defined diameter to open up intergranular fissures.
  • Visual examination: inspecting the tension surface of the bent specimen at defined magnification for cracks, fissures, or delamination.
  • Metallographic examination (arbitration): when visual results are questionable, preparing a cross-section of the bent specimen and microscopically measuring the depth of intergranular attack to confirm or reject the presence of IGC.
  • Supplementary screening test: electrolytic etching in oxalic acid per ASTM A262 Practice A or equivalent, used to classify etch structures and potentially exempt "step" structures from further testing.

Testing Methods

The most common procedure associated with the bend test is the copper–copper sulfate–sulfuric acid test (Strauss test), specified in ASTM A262 Practice E, ISO 3651-2 Method A, and GB/T 4334 Method E. The general workflow is as follows:

  • Specimen preparation: specimens are degreased, descaled if necessary, measured, weighed where required, and identified.
  • Test solution preparation: the solution contains copper sulfate (CuSO4·5H2O) and sulfuric acid (H2SO4) in distilled or deionized water — for the 16% sulfuric acid variant, typically 100 g/L CuSO4·5H2O with 16% H2SO4 by weight percentage as defined in the standard.
  • Exposure: specimens are placed in contact with metallic copper chips or shot in the boiling solution for the specified duration, commonly 24 hours for the 16% sulfuric acid method (16 hours for the 50% sulfuric acid variant, 20 hours for the 35% variant, per ISO 3651-2).
  • Rinsing and drying: after exposure, specimens are rinsed, dried, and visually inspected for gross attack.
  • Bend test: the specimen is bent through 180° (or the angle specified in the product specification) around a mandrel with a diameter generally not greater than the specimen thickness, using a bend apparatus, press, or vise with rounded jaws.
  • Evaluation: the convex (tension) surface is examined for cracking. The appearance of cracks visible to the unaided eye or under low magnification indicates intergranular corrosion susceptibility. When results are doubtful, a metallographic cross-section perpendicular to the bend is examined to determine whether cracks are attributable to intergranular attack or to other causes such as mechanical tearing.

Alternative immersion environments used in conjunction with bend or mass-loss evaluation include the ferric sulfate–sulfuric acid test (ASTM A262 Practice B, ASTM G28 Practice A, ISO 3651-2 Method C), the nitric acid Huey test (ASTM A262 Practice C, ISO 3651-1), and the copper–copper sulfate–50% sulfuric acid test (ASTM A262 Practice F, ISO 3651-2 Method B). The choice of method depends on the steel grade, the corrosion environment anticipated in service, and the requirements of the purchase specification. Ferritic and duplex stainless steels are typically evaluated using ASTM A763 or ASTM G28, respectively, since the Strauss-type test is not equally sensitive to all microstructural conditions.

Applications

Intergranular corrosion bend testing is applied extensively across industries where the structural integrity of stainless steel components must be guaranteed in aggressive environments:

  • Petrochemical and chemical processing: pressure vessels, heat exchangers, reactors, and piping handling acidic media where weld sensitization could initiate intergranular failure.
  • Nuclear power: reactor internals, cooling circuits, and containment components requiring rigorous qualification of austenitic stainless steels against irradiation-assisted and thermal sensitization.
  • Oil and gas: offshore platforms, subsea pipelines, and refining equipment exposed to chloride- and sulfur-containing environments.
  • Food and beverage processing: sanitary tubing, tanks, and equipment that undergo repeated welding and must maintain corrosion resistance and cleanliness.
  • Pharmaceutical and biotechnology: high-purity process systems fabricated from low-carbon or stabilized austenitic grades, verified by IGC testing after fabrication.
  • Pulp and paper: digesters, bleach plant equipment, and liquor handling systems exposed to hot acidic liquors.
  • Material qualification and acceptance testing: mill products, forgings, castings, and welded consumables supplied to specifications referencing ASTM, ISO, EN, or GB standards.
  • Failure analysis and research: investigating service failures attributed to sensitization and developing new alloys or welding procedures with improved resistance to intergranular attack.

FAQ

What causes intergranular corrosion in stainless steel?

Intergranular corrosion is caused by chromium carbide precipitation at grain boundaries when the steel passes through the sensitization temperature range of approximately 425 °C to 815 °C, commonly encountered during welding or improper heat treatment. The chromium-depleted zones adjacent to the grain boundaries lose passivity and dissolve preferentially in specific corrosive media.

How can sensitization be prevented?

Sensitization can be prevented by selecting low-carbon grades (for example, 304L or 316L with carbon content ≤ 0.03%), stabilized grades containing titanium or niobium (such as 321 or 347), applying solution annealing after fabrication, or controlling welding heat input and cooling rates.

Why is a bend test performed after the corrosion exposure?

The corrosion immersion itself may leave the specimen visually unchanged because intergranular attack is localized at the microscopic level. Bending the specimen places the tension surface under tensile stress, which opens up embrittled grain boundaries and renders intergranular cracks visible for evaluation, making the bend test a simple yet sensitive acceptance criterion.

What bend angle and mandrel diameter are used?

Most standards specify a 180° bend around a mandrel whose diameter is equal to or not greater than the specimen thickness, although product specifications may define other angles or bend radii depending on material thickness and grade.

What is the difference between the Strauss, Huey, and ferric sulfate tests?

The Strauss test (copper–copper sulfate–sulfuric acid) primarily detects chromium depletion from carbide precipitation and is the method most commonly paired with the bend test. The Huey test (boiling nitric acid) is more severe and also detects sigma phase and other nitric-acid-selective phases. The ferric sulfate–sulfuric acid test is a mass-loss method sensitive to chromium-depleted regions and certain secondary phases, evaluated by corrosion rate rather than bending.

What should be done if the bent specimen shows cracks?

Cracks observed on the bend tension surface indicate probable intergranular attack, but the result should be confirmed metallographically by examining a cross-section of the bent specimen at magnification. If intergranular cracks are confirmed, the material is rejected for the intended application, and corrective actions such as solution annealing, requalification of welding procedures, or material replacement should be considered.

How long does the test take?

The boiling immersion typically lasts 24 hours for the 16% sulfuric acid Strauss method, with additional time required for specimen preparation, sensitization heat treatment where specified, bend testing, and metallographic confirmation if needed. The total turnaround commonly ranges from three to seven working days depending on the scope of testing defined with the accredited third-party laboratory.